紫外穩(wěn)定。 良好的清晰度、耐熱性、性能保留性、尺寸穩(wěn)定性。
TYPICAL PROPERTIES (1) | |||
MECHANICAL/機(jī)械性能
|
Value/值 | Unit/單位 | Standard/標(biāo)準(zhǔn) |
Tensile Stress, yld, Type I / 抗張程度,屈服,類型I, 50 mm/min
|
62
|
MPa
|
ASTM D 638
|
Tensile Stress, brk, Type I / 抗張程度,斷裂,類型I, 50 mm/min
|
65
|
MPa
|
ASTM D 638
|
Tensile Strain, brk, Type I / 拉伸伸長(zhǎng),斷裂,類型I, 50 mm/min
|
110
|
%
|
ASTM D 638
|
Flexural Stress, yld / 撓曲強(qiáng)度, 屈服 , 1.3 mm/min, 50 mm span
|
93
|
MPa
|
ASTM D 790
|
Flexural Modulus / 撓曲模量, 1.3 mm/min, 50 mm span
|
2300
|
MPa
|
ASTM D 790
|
IMPACT/沖擊性能
|
Value/值 | Unit/單位 | Standard/標(biāo)準(zhǔn) |
Izod Impact, notched / 懸臂梁缺口沖擊強(qiáng)度, 23°C
|
640
|
J/m
|
ASTM D 256
|
Tensile Impact Type / 拉伸沖擊值,類型”S”
|
378
|
kJ/m2
|
ASTM D 1822
|
Instrumented IMPACT Energy @ peak / 儀表控制抗沖擊能量 @ 峰值, 23°C
|
54
|
J
|
ASTM D 3763
|
THERMAL/熱性能
|
Value/值 | Unit/單位 | Standard/標(biāo)準(zhǔn) |
HDT(熱變形溫度), 1.82 MPa, 6.4 mm, unannealed (未退火)
|
126
|
°C
|
ASTM D 648
|
Relative Temp Index, Elec / 相對(duì)熱指數(shù), 電性能
|
130
|
°C
|
UL 746B
|
Relative Temp Index, Mech w/impact / 相對(duì)熱指數(shù),機(jī)械沖擊性能
|
130
|
°C
|
UL 746B
|
Relative Temp Index, Mech w/o impact / 相對(duì)熱指數(shù),非機(jī)械沖擊性能
|
130
|
°C
|
UL 746B
|
PHYSICAL/物理性能
|
Value/值 | Unit/單位 | Standard/標(biāo)準(zhǔn) |
Specific Gravity / 比重
|
1.2
|
–
|
ASTM D 792
|
Mold Shrinkage / 收縮率, flow(流動(dòng)), 3.2 mm
|
0.5 – 0.7
|
%
|
SABIC bbbbbb
|
Melt Flow Rate / 熔流率,, 300°C/1.2 kgf
|
25
|
g/10 min
|
ASTM D 1238
|
OPTICAL/光學(xué)性能
|
Value/值 | Unit/單位 | Standard/標(biāo)準(zhǔn) |
Light Transmission / 透光率
|
88
|
%
|
ASTM D 1003
|
Haze / 霧度
|
1
|
%
|
ASTM D 1003
|
FLAME CHARACTERISTICS/火焰特性
|
Value/值 | Unit/單位 | Standard/標(biāo)準(zhǔn) |
UL Recognized, 94V-2 Flame Class Rating / 阻燃等級(jí) (3)
|
1.2
|
mm
|
UL 94
|
CSA (See File for complete listing)
|
LS88480
|
File No.
|
CSA LISTED
|
Processing/加工方法
|
Parameter | ||
Injection Molding/注塑參數(shù)
|
Value/值 | Unit/單位 |
Drying Temperature / 干燥溫度
|
120
|
°C
|
Drying Time / 干燥時(shí)間
|
3 – 4
|
hrs
|
Drying Time (Cumulative) / 干燥時(shí)間(累積的)
|
48
|
hrs
|
Maximum Moisture Content / 最大含濕量
|
0.02
|
%
|
Melt Temperature / 熔體溫度
|
270 – 295
|
°C
|
Nozzle Temperature / 注嘴溫度
|
265 – 290
|
°C
|
Front – Zone 3 Temperature / 前區(qū)3溫度
|
270 – 295
|
°C
|
Middle – Zone 2 Temperature / 中區(qū)2溫度
|
260 – 280
|
°C
|
Rear – Zone 1 Temperature / 后區(qū)1溫度
|
250 – 270
|
°C
|
Mold Temperature / 模具溫度
|
70 – 95
|
°C
|
Back Pressure / 背壓
|
0.3 – 0.7
|
MPa
|
Screw Speed / 螺桿速度
|
40 – 70
|
rpm
|
Shot to Cylinder Size / 每次注射量占料筒熔膠總量的百分比
|
40 – 60
|
%
|
Vent Depth / 排氣孔深度
|
0.025 – 0.076
|
mm
|